Reference standard: EN 12591:2009
| Property | Unit | Method | PARAFALT ASF 20/30
 
 | PARAFALT ASF 30/45
 
 | PARAFALT ASF 35/50
 
 | 
|---|
| Penetration at 25°C | 0,1 mm | EN 1426 | 20-30 | 30-45 | 35-50 | 
| Softening Point R&B | ºC | EN 1427 | 55-63 | 52-60 | 50-58 | 
| Retained penetration at 25°C | % | EN 12607-1EN 1426
 | ≥ 55 | ≥ 53 | ≥ 53 | 
| Increasing of Softening Point R&B | ºC | EN 12607-1EN 1427
 | ≤ 10 | ≤ 11 | ≤ 11 | 
| Mass change after RTFOT | % | EN 12607-1 | ≤ 0,5 | ≤ 0,5 | ≤ 0,5 | 
| Flash point, COC | ºC | EN ISO 2592 | ≥ 240 | ≥ 240 | ≥ 240 | 
| Solubility | % | EN 12592 | ≥ 99,0 | ≥ 99,0 | ≥ 99,0 | 
| Fraass breaking point | ºC | EN 12593 | - | ≤ -5 | ≤ -5 | 
 
| Properties | Unit | Method | PARAFALT ASF 50/70
 
 | PARAFALT ASF 70/100
 
 | PARAFALT ASF 100/150
 
 | 
|---|
| Penetration at 25°C | 0,1 mm | EN 1426 | 50-70 | 70-100 | 100-150 | 
| Softening Point R&B | ºC | EN 1427 | 46-54 | 43-51 | 39-47 | 
| Retained penetration at 25°C | % | EN 12607-1EN 1426
 | ≥ 50 | ≥ 46 | ≥ 43 | 
| Increasing of Softening Point R&B | ºC | EN 12607-1EN 1427
 | ≤ 11 | ≤ 11 | ≤ 12 | 
| Mass change after RTFOT | % | EN 12607-1 | ≤ 0,5 | ≤ 0,8 | ≤ 0,8 | 
| Flash point, COC | ºC | EN ISO 2592 | ≥ 230 | ≥ 230 | ≥ 230 | 
| Solubility | % | EN 12592 | ≥ 99,0 | ≥ 99,0 | ≥ 99,0 | 
| Fraass breaking point | ºC | EN 12593 | ≤ -8 | ≤ -10 | ≤ -12 | 
| Properties | Unit | Method | PARAFALT  ASF 160/220
 
 | 
|---|
| Penetration at 25°C | 0,1 mm | EN 1426 | 160-220 | 
| Softening Point R&B | ºC | EN 1427 | 35-43 | 
| Retained penetration at 25°C | % | EN 12607-1EN 1426
 | ≥ 37 | 
| Increasing of Softening Point R&B | ºC | EN 12607-1EN 1427
 | ≤ 12 | 
| Mass change after RTFOT | % | EN 12607-1 | ≤ 1,0 | 
| Flash point, COC | ºC | EN ISO 2592 | ≥ 220 | 
| Solubility | % | EN 12592 | ≥ 99,0 | 
| Fraass breaking point | ºC | EN 12593 | ≤ -15 |