Reference standard: EN 12591:2009
| Properties | 
Unit | 
Method | 
50/70 | 
70/100 | 
160/220 | 
| Penetration at 25°C | 
0,1 mm | 
EN 1426 | 
50-70 | 
70-100 | 
160-220 | 
| Softening Point R&B | 
ºC | 
EN 1427 | 
46-54 | 
43-51 | 
35-43 | 
| Retained penetration at 25°C | 
% | 
EN 12607-1 EN 1426  | 
≥ 50 | 
≥ 46 | 
≥ 37 | 
| Increasing of Softening Point R&B | 
ºC | 
EN 12607-1 EN 1427  | 
≤ 11 | 
≤ 11 | 
≤ 12 | 
| Mass change after RTFOT | 
% | 
EN 12607-1 | 
≤ 0,5 | 
≤ 0,8 | 
≤ 1,0 | 
| Flash point, COC | 
ºC | 
EN ISO 2592 | 
≥ 230 | 
≥ 230 | 
≥ 220 | 
| Solubility | 
% | 
EN 12592 | 
≥ 99,0 | 
≥ 99,0 | 
≥ 99,0 | 
| Fraass breaking point | 
ºC | 
EN 12593 | 
≤ -8 | 
≤ -10 | 
≤ -15 | 
*) Requirementin Poland: PN-EN 12591:2010